<p id="httnz"></p>
<video id="httnz"></video><p id="httnz"></p>

<p id="httnz"><output id="httnz"><font id="httnz"></font></output></p><p id="httnz"></p>

<p id="httnz"></p>
<video id="httnz"><output id="httnz"><font id="httnz"></font></output></video>
<p id="httnz"><output id="httnz"><font id="httnz"></font></output></p>
<video id="httnz"></video>

<p id="httnz"></p>
<video id="httnz"><output id="httnz"><font id="httnz"></font></output></video>
<p id="httnz"><output id="httnz"></output></p>

<video id="httnz"></video>

<p id="httnz"><output id="httnz"></output></p>
<p id="httnz"><output id="httnz"><delect id="httnz"></delect></output></p>

<p id="httnz"></p>

<video id="httnz"></video>
<video id="httnz"><p id="httnz"></p></video>
<p id="httnz"><output id="httnz"></output></p>
<video id="httnz"><p id="httnz"></p></video>
<p id="httnz"></p><video id="httnz"><output id="httnz"><font id="httnz"></font></output></video><video id="httnz"><p id="httnz"><font id="httnz"></font></p></video><video id="httnz"><output id="httnz"></output></video><video id="httnz"><output id="httnz"><delect id="httnz"></delect></output></video><video id="httnz"><output id="httnz"><delect id="httnz"></delect></output></video>
<video id="httnz"></video> <p id="httnz"></p>
<p id="httnz"></p>
<video id="httnz"><output id="httnz"></output></video>

<video id="httnz"><output id="httnz"><delect id="httnz"></delect></output></video>

<video id="httnz"></video>

<p id="httnz"><output id="httnz"></output></p>
<p id="httnz"><video id="httnz"><delect id="httnz"></delect></video></p>

精品軸承鋼管
軸承鋼管廠
您的位置:首頁 > 新聞中心 > 技術資訊

遼河油田高效液壓套管整形工具的研制與應用

2021-10-09

遼河油田高效液壓套管整形工具的研制與應用

張洪寶1,2

(1.中國石油遼河油田分公司鉆采工藝研究院,遼寧盤錦 124010;2.東北石油大學石油工程學院,黑龍江大慶 163318)

摘 要:針對遼河油田變形套管整形修復率低、施工周期長及成本高的問題,根據液力增壓和滾珠擠壓整形原理,研制了高效液壓套管整形工具。該整形工具由整形頭、增壓液缸、泄壓裝置和液壓錨定裝置構成。室內試驗表明:液壓套管整形工具的整形效率高,與常規整形工具相比,整形效率提高約40%,且對套管損傷小,能盡可能恢復套管內徑。該整形工具在遼河油田13口套損井進行了現場應用,順利完成了12口井的套管修復,成功率92.3%。研究與應用表明,液壓套管整形工具適用于套管縮徑井的修復作業,能基本滿足遼河油田套損井套管整形的需要。

關鍵詞:套管損壞;套管整形;杜80-30-58井;遼河油田

目前,遼河油田共有停產井近2 800 口,并且以平均每年10%的比例上升。其中因套管損壞而停產的井約占35%,現有套損井1 000 多口,每年還會增加200多口新套損井。截至2015年底,僅修復套損井306口,大部分套損井亟待修復。遼河油田套損類型以套管變形為主,占總套損井的80%[1]。遼河油田現有的套損井套管整形技術主要有機械整形和爆炸整形兩類,且均存在缺陷:機械整形中梨形器擴脹技術、套管磨銑技術和偏心輥子整形技術等普遍存在著損傷套管、犧牲套管厚度、難以恢復原通徑等問題;爆炸整形技術的用藥量很難把握,變形處的套管壁厚不均,由于爆炸沒有方向性不可避免會對套管造成破壞。原來的套管整形技術修復成功率低、施工周期長、成本高,遠不能滿足遼河油田套損井套管整形修復的需要。為此,針對遼河油田套損井的實際情況,根據液力增壓和滾珠擠壓整形原理[2-5],研制了整形效率高、對套管損傷小、結構緊湊、性能可靠的液壓套管整形工具,并對13 口套損井進行了套管修復,成功率92.3%,提高了遼河油田套損井的修復效率及效果。

1 液壓套管整形工具的結構與工作原理

液壓套管整形工具的研制思路是將壓井液的液壓能轉化成機械能,推動滾珠克服套管和巖石的變形應力和擠壓力,使套管向外擴展產生膨脹,迫使地應力在局部范圍內重新分布,達到整形的目的。

1.1 結構

液壓套管整形工具由整形頭、增壓液缸(三級)、錨定裝置和泄壓裝置構成,如圖1所示。

整形頭是圓錐形結構,其上設有球槽,球槽是帶有坡度的燕尾槽,大小2種數十個整形球卡在球槽內,并用穩釘限位,整形球在整形槽內可以上下自由移動,如圖2所示。工作時整形器在液壓作用下向下運動,整形球上移至球槽最上端,此時整形頭最大外徑158.0 mm;一個整形周期結束后,泄壓上提管柱,整形球下移至球槽最下端,此時整形頭最大外徑150.0 mm;整形完畢后整形頭外徑回縮8.0 mm,能夠有效防止卡管柱事故的發生,同時將管柱之間的面摩擦轉變成滾動摩擦,大大減小了上提管柱時的摩擦阻力[6-7]。

圖1 液壓套管整形工具的整體結構
Fig.1 The overall structure of the hydraulic casing restoration tool


圖2 整形頭的基本結構
Fig.2 The basic structure of the shaping head

增壓液缸為直線式結構,工作時從工具上部加壓,使下部的球閥坐到閥座上密封本體腔,同時流體從中心管液流孔流出,推動中心管接頭帶動整個工具向下運動,實現快速有效地為下部工具增加液壓動力的目的。在25 MPa壓差作用下,單級液缸可產生200 kN的上推力,根據現場需要,可以任意組裝3~6級,上推力可達到600~1 200 kN。

泄壓裝置主要由內、外2個中心管組成,其上設有液流孔。正常工作時,下壓管柱將內、外中心管上的液流孔錯開,泄壓裝置本體腔成密閉環境;一個整形周期完成后需要泄壓時,上提管柱,將內、外中心管上的液流孔對齊,泄壓裝置本體腔內的流體經泄壓孔流到管柱外,實現安全泄壓。

1.2 工作原理

工作時,首先用管柱將整形工具下至井下套管變形部位,加壓推出錨定裝置的錨爪,將整形工具錨定在套管內壁上,阻止上部鉆具下移,實現對錨定裝置上部管柱和修井設備的有效保護。繼續加壓,推動整形工具向下移動,整形頭上的整形球滾動擠壓套損部位,使套管直徑逐漸恢復。套管變形的恢復是逐級進行的,首先整形頭下部的小直徑整形球先接觸套管變形部位,對其滾壓,隨著整形工具的下移,整形球沿楔形球槽上移,整形工具的直徑隨之變大,逐步修復變形套管;小直徑整形球通過套管變形部位后,整形頭上部的大直徑整形球開始滾壓套管變形部位,隨著整形工具的繼續下移,大直徑整形球沿楔形球槽上移,工具直徑隨之變大,進一步修復變形套管,直至大直徑整形球通過套管變形部位,套管直徑恢復到預先設計的尺寸,完成套管修復。整形過程中,通過增壓液缸增大整形頭向下的擠壓力,提高了工作效率。整形結束后通過泄壓裝置卸掉管柱內的壓力,解除錨定,即可上提管柱,起出整形工具[8-10]。

該整形工具一次整形的最大長度為390 mm,當套管變形部位長度大于390 mm時,需進行多次整形,即一次整形結束后泄壓解除錨定,下放管柱,重復上述整形過程。

1.3 主要技術參數

液壓套管整形工具長6 200 mm,最大外徑158.0 mm,一次行程400 mm,耐溫260 ℃,承壓40 MPa。整形頭材質35CrMo,公稱外徑142.2 mm,整形球材質9Cr18Mo,大球直徑20.0 mm,小球直徑15.0 mm;增壓液缸材質35CrMo,外徑146.1 mm;泄壓裝置材質35CrMo,外徑146.1 mm;錨定裝置材質35CrMo,外徑146.1 mm。

1.4 技術特點

1) 對套管損壞小。利用整形鋼球的滾動使套管變形部位逐漸恢復原狀,套管直徑的恢復是逐級實現的,對套管損壞較小。

2) 整形效率高。在25 MPa壓差作用下,整形動力最高可達到1 200 kN,且采用鋼球滾動擠壓整形,摩擦阻力小,整形速度快、效率高。

3) 泄壓方便。泄壓裝置由內、外2個中心管組成,整形時內、外中心管上的泄壓孔錯開,泄壓裝置本體腔為密閉環境;整形結束后上提管柱,內、外中心管上的泄壓孔對齊,實現安全泄壓。

4) 有效防卡。整形時整形工具的外徑達到158.0 mm,而整形結束后整形工具外徑回縮8.0 mm,能有效防止卡管柱事故的發生。

2 室內試驗

為了檢驗液壓套管整形工具的技術指標和整形效果是否達到設計要求,在室內進行了整形模擬試驗。

2.1 試驗器材

液壓套管整形工具;試驗平臺;加壓設備;高壓管線、數顯壓力表、游標卡尺、吊車、管鉗、扳手等工具;φ177.8 mmP110鋼級套管,套管有2處縮徑,縮徑方向與套管中心軸線基本垂直[11-12]。

2.2 試驗步驟

1) 測量φ177.8 mm套管縮徑處的外徑分別為139.7 mm和145.3 mm,變形長度分別為260 mm和512 mm。

2) 連接好液壓套管整形工具及液壓管線,加壓驗證整形工具和液壓管線的密封是否可靠。

3) 將連接好的整形工具送入φ177.8 mm套管內,當整形頭到達套管縮徑處時,加壓錨定整形工具后,繼續加壓對縮徑處實施整形。完成套管第1縮徑處整形后,泄壓,順利起出管柱。

4) 對第2縮徑處進行整形,整形長度達到一次整形長度極限(390 mm)后泄壓,繼續對第2縮徑處進行整形,直至通過第2縮徑處。

5) 泄壓后起出管柱,測量并記錄套管整形后的內外徑,觀察套管變形反彈情況。

2.3 試驗結果

1) 第1縮徑處整形用時14.5 min,第2縮徑處整形用時34.5 min,整形速度約0.94 m/h,而套管變形一般在20 m以內,采用常規整形技術需要36.0 h(整形速度約0.56 m/h),與之相比,液壓套管整形工具的整形效率提高約40%。

2) φ177.8 mm套管的2個縮徑處完成整形后,外徑達到170.7 mm,內徑恢復到158.0 mm。

3) 整形結束后,套管變形處內徑有所回縮,60 min內的回縮最大值為2.5 mm,但沒有超過整形工具整形頭球槽上下4.0 mm的高度差,試驗中取出工具時沒有明顯阻力,說明該工具能夠有效防止卡管柱現象的發生。

3 現場應用

截至目前,液壓套管整形工具在13 口井進行了應用,成功完成12口套損井的修復,成功率達92.3%,基本解決了遼河油田套管變形修復成功率低的難題。下面以杜80-30-58井為例介紹該工具的現場應用情況。

杜80-30-58井井深為1 050.00 m,最大井斜角為11.87°(井深885.00 m處)。該井套管程序為φ273.0 mm套管×103.94 m+φ177.8 mm套管×1 056.81 m,水泥返高812.17 m。該井在修井作業時,通井至井深851.88 m遇阻,下φ154.0 mm鉛模打印,鉛模穿過,根據鉛模顯示的信息確定井深851.88 m處φ177.8 mm套管縮徑至150.0 mm,于是采用液壓套管整形工具進行整形,以便順利完成修井作業。套管整形步驟為:

1) 利用油管將液壓套管整形工具送到井下,當整形工具下到套管縮徑處,遇阻,說明整形工具的整形頭已經接觸到了套變部位;

2) 調整油管柱長度,將油管上端與泵車水管接頭連接起來;

3) 檢驗并準確調整油管柱,并在井口油管柱做標記;

4) 將懸重歸零,用作業機將管柱吊住并適當放松;

5) 將油管柱注滿水,緩慢加壓至20~25 MPa,穩壓2~3 min;

6) 上拉油管柱,打開泄壓開關,泄掉油管柱內的水;泄壓后油管柱下行約250~300 mm,即套管整形修復長度為250~300 mm;

7) 重復上述步驟,先后經過6次修復,將套管縮徑部位全部整形完畢。

該井完成套管整形后,起出油管柱和液壓套管整形工具,下入φ151.6 mm通井規通井至人工井底,無遇阻現象,隨后順利完成修井作業。

4 結 論

1) 根據遼河油田實際情況,研制了高效液壓套管整形工具,該工具具有對套管損傷小、整形效率高、泄壓方便和有效防卡的優點。

2) 室內模擬試驗表明,高效液壓套管整形工具整形速度快、效率高,其整形速度比常規整形工具高40%左右。

3) 高效液壓套管整形工具在遼河油田13口套損井的套管修復過程中未出現任何事故,整形效果顯著,成功率達92.3%。

4) 高效液壓套管整形工具對單點或多點縮徑套管的修復效果較好,對其他類型套損的修復還需要進行研究。

參 考 文 獻:

[1] 李海軍.遼河油田套損機理及防治建議[J].內蒙古石油化工,2012,22(3):57-59.

LI Haijun.The mechanism and prevention of casing damage in Liaohe Oilfield[J].Inner Mongulia Petrochemical Industry,2012,22(3):57-59.

[2] 翟曉鵬,樓一珊,周建良,等.套管徑向變形可修復界限研究[J].石油鉆探技術,2012,40(1):28-31.

ZHAI Xiaopeng,LOU Yishan,ZHOU Jianliang,et al.Study of minimum repair limit for reduced casing deformation[J].Petroleum Drilling Techniques,2012,40(1):28-31.

[3] 王小增,楊久紅,竇益華.套管磨損后剩余壁厚及剩余強度分析[J].石油鉆探技術,2008,36(2):14-17.

WANG Xiaozeng,YANG Jiuhong,DOU Yihua.Analysis of casing remaining thickness and residual strength after wearing[J].Petroleum Drilling Techniques,2008,36(2):14-17.

[4] 闞慶山,劉汝東,蘇娟.套損井修復技術在中原油田的應用[J].斷塊油氣田,2009,16(3):121-122.

KAN Qingshan,LIU Rudong,SU Juan.Application of repairing technology for casing damage well in Zhongyuan Oilfield[J].Fault-Block Oil & Gas Field,2009,16(3):121-122.

[5] 竇益華,張福祥,王維君,等.井下套管磨損深度及剩余強度分析[J].石油鉆采工藝,2007,29(4):36-39.

DOU Yihua,ZHANG Fuxiang,WANG Weijun,et al.Analysis on wear depth and residual strength of downhole casing[J].Oil Drilling & Production Technology,2007,29(4):36-39.

[6] 梁爾國,李子豐,趙金海.磨損套管抗擠強度計算模型[J].石油鉆探技術,2012,40(2):41-45.

LIANG Erguo,LI Zifeng,ZHAO Jinhai.Model for collapsing strength calculation of worn casing[J].Petroleum Drilling Techniques,2012,40(2):41-45.

[7] 王維星,武瑞霞,李在訓,等.液壓變徑滾壓套管整形技術[J].石油機械,2010,38(7):86-87.

WANG Weixing,WU Ruixia,LI Zaixun,et al.Hydraulic variable diameter rolling sleeve shaping technique[J].China Petroleum Machinery,2010,38(7):86-87.

[8] 房育金,郭偉鋒,張云杰,等.低滲透油田套管損壞機理分析及防治措施[J].特種油氣藏,2006,13(4):78-80.

FANG Yujin,GUO Weifeng,ZHANG Yunjie,et al.Casing failure mechanism analysis and prevention measures[J].Special Oil & Gas Reservoirs,2006,13(4):78-80.

[9] 田玉剛,皇甫潔,李華彬.套變井液壓整形技術研究[J].勝利油田職工大學學報,2009,23(3):45-46,48.

TIAN Yugang,HUANGFU Jie,LI Huabin.Study on the hydraulic shaping technology of the casing damage well[J].Journal of Shengli Oil Field Staff University,2009,23(3):45-46,48.

[10] 何育榮,朱海波.膨脹篩管的研制及現場試驗[J].石油鉆探技術,2011,39(3):106-109.

HE Yurong,ZHU Haibo.Expansion sand screen development and field test[J].Petroleum Drilling Techniques,2011,39(3):106-109.

[11] 關舒偉,李春福,李學藝,等.非均勻外擠壓力作用下內徑偏磨套管的應力分析[J].石油鉆探技術,2009,37(2):38-40.

GUAN Shuwei,LI Chunfu,LI Xueyi,et al.Stress analysis of worn casing under heterogeneous external pressure[J].Petroleum Drilling Techniques,2009,37(2):38-40.

[12] 宋根才.復雜井況水平井套管損壞機理及預防技術研究[D].東營:中國石油大學(華東)機電工程學院,2010.

SONG Gencai.Study on casing damage mechanism and prevention[D].Dongying:China University of Petroleum(Huadong),College of Mechanical and Electronic Engineering,2010.

[編輯 劉文臣]

The Development and Application of a High Efficiency Hydraulic Casing Restoration Tool

ZHANG Hongbao1,2

(1.Drilling & Production Technology Research Institute, PetroChina Liaohe Oilfield Company, Panjin, Liaoning, 124010, China; 2. School of Petroleum Engineering, Northeast Petroleum University, Daqing, Heilongjiang, 163318, China)

Abstract:At present, operations related to the restoration of deformed casing in the Liaohe Oilfield can be characterized by low success rates, long operation duration and high costs. Based on the principles of hydraulic boosting and rolling ball squeezing, a high efficiency hydraulic casing restoration tool has been developed, which is composed of a shaping head, pressure cylinder, pressure relief device and hydraulic anchoring device. Experimental results showed that the hydraulic casing shaping tool possessed high shaping efficiency, the average single well restoration duration was reduced by 40% from the original state. With less damage to the casing, the newly developed tool could be used to achieve maximum restoration of inner size of the casing. This tool has been used in the casing restoration of 13 wells in the Liaohe Oilfield and experienced success in 12 wells, resulting in a success rate of 92.3%. Both research results and application performances showed that the hydraulic casing restoration tool could be used for casing restoration of wells with deformed casing to meet the demands for casing re-shaping in the Liaohe Oilfield.

Key words:casing damage; hydraulic casing restoration; Well Du-80-30-58; Liaohe Oilfield

 

精品軸承鋼管廠

欧美精品亚洲精品日韩传电影
<p id="httnz"></p>
<video id="httnz"></video><p id="httnz"></p>

<p id="httnz"><output id="httnz"><font id="httnz"></font></output></p><p id="httnz"></p>

<p id="httnz"></p>
<video id="httnz"><output id="httnz"><font id="httnz"></font></output></video>
<p id="httnz"><output id="httnz"><font id="httnz"></font></output></p>
<video id="httnz"></video>

<p id="httnz"></p>
<video id="httnz"><output id="httnz"><font id="httnz"></font></output></video>
<p id="httnz"><output id="httnz"></output></p>

<video id="httnz"></video>

<p id="httnz"><output id="httnz"></output></p>
<p id="httnz"><output id="httnz"><delect id="httnz"></delect></output></p>

<p id="httnz"></p>

<video id="httnz"></video>
<video id="httnz"><p id="httnz"></p></video>
<p id="httnz"><output id="httnz"></output></p>
<video id="httnz"><p id="httnz"></p></video>
<p id="httnz"></p><video id="httnz"><output id="httnz"><font id="httnz"></font></output></video><video id="httnz"><p id="httnz"><font id="httnz"></font></p></video><video id="httnz"><output id="httnz"></output></video><video id="httnz"><output id="httnz"><delect id="httnz"></delect></output></video><video id="httnz"><output id="httnz"><delect id="httnz"></delect></output></video>
<video id="httnz"></video> <p id="httnz"></p>
<p id="httnz"></p>
<video id="httnz"><output id="httnz"></output></video>

<video id="httnz"><output id="httnz"><delect id="httnz"></delect></output></video>

<video id="httnz"></video>

<p id="httnz"><output id="httnz"></output></p>
<p id="httnz"><video id="httnz"><delect id="httnz"></delect></video></p>